Flexible Pavement Structural Number
Each layer spreads the wheel load a little wider, and the structural number adds up their contributions.
Before this Lesson
- Traffic Loading and ESALs
- Asphalt Concrete · Materials
Walk across deep snow in boots and you sink to your knees. Strap on snowshoes and you stay near the top. You weigh the same either way; the snowshoes just hand your weight to the snow over a bigger area, so each square inch of snow carries less.
A loaded truck tire presses on the road at about its inflation pressure, roughly 100 psi, through a patch not much bigger than your hand. The soil under the road would soon rut under that, pass after pass. A flexible pavement is a stack of snowshoes between the two, and the structural number is how you add up what the stack can do.
Each layer spreads the load wider
A typical flexible pavement puts three layers on top of the natural soil, which is called the subgrade:
- an asphalt concrete surface, the rock skeleton glued and sealed by binder from Asphalt Concrete;
- a base of compacted crushed stone, with no binder;
- a subbase of cheaper gravel or sand.
Each layer receives the load on a small area at its top and hands it down over a larger area at its bottom. By the time the load reaches the subgrade, it covers many times the area of the tire's patch, and the pressure is a small fraction of 100 psi.
How far a layer spreads the load depends on how stiff it is. Press a coin into a foam pad and only the foam right under the coin squashes. Lay a stiff board on the pad and press the same coin on the board, and the whole pad under the board shares the load. A stiff layer is the board. An inch of asphalt concrete spreads the load farther than an inch of crushed stone, which spreads it farther than an inch of gravel or sand.
That's why the layers come in this order. The pressure is highest right under the tire, so the stiffest and most expensive material goes on top, where it does the most good, and cheaper material goes lower, where the load has already spread out. The stack is called flexible because it bends a little under every wheel and springs back, instead of bridging the load the way a stiff concrete slab does.
The structural number adds up the stack
AASHTO's method boils the whole stack down to one number, the structural number , an index of the pavement's total load-spreading capacity. It isn't a thickness, and you can't measure it with a ruler. It's each layer's thickness, weighted by how good that material is at spreading load, all added up.
The weight is the layer coefficient , the structural number that one inch of a material adds. The classic values come from the same AASHO Road Test as the load equivalency factors in Traffic Loading and ESALs: about 0.44 for asphalt concrete, 0.14 for a crushed-stone base, and 0.11 for a sandy gravel subbase. Asphalt concrete's is the highest, and an inch of it is worth about three inches of base. The Handbook prints no layer coefficients, so a question gives them.
Leaving drainage aside for the moment, each layer contributes its coefficient times its thickness in inches. For 4 in of asphalt concrete over 10 in of base and 12 in of subbase:
A design starts from the structural number the pavement needs. AASHTO's design equation takes the design ESALs, the subgrade's stiffness, and how reliable the agency wants the pavement to be, and returns the required SN. More trucks or a weaker subgrade call for a larger one. The Handbook doesn't print that equation, so on the exam the required SN is given, and your job is the stack.
Water weakens the base
The asphalt surface is held together by its binder. The base and subbase are unbound: nothing glues them, and they hold their shape only because their stones press and grind against each other. Water undermines that. When the voids fill with water, each passing wheel squeezes the layer faster than the water can get out, so for that instant the water carries part of the load and the stones press together less. Fines mix with the water into a slurry that lubricates the contacts. A wet base is a softer base.
So AASHTO discounts the two unbound layers with a drainage coefficient , which multiplies each one's contribution. Two things set it: how quickly water drains out of the layer, and how much of the year the layer spends near saturation. AASHTO's design guide tabulates it, and the Handbook doesn't, so here is a reduced version.
| Drainage | Water drains in | Under 1% | Over 25% |
|---|---|---|---|
| Excellent | 2 hours | 1.35–1.40 | 1.20 |
| Good | 1 day | 1.25–1.35 | 1.00 |
| Fair | 1 week | 1.15–1.25 | 0.80 |
| Poor | 1 month | 1.05–1.15 | 0.60 |
| Very poor | Doesn't drain | 0.95–1.05 | 0.40 |
Adapted from the AASHTO Guide for Design of Pavement Structures, 1993
Read across a row and the coefficient falls as the layer spends more of the year wet. Read down a column and it falls as drainage gets worse. Notice that 1.0 is middling, not perfect, and it's the Handbook's default: assume unless a question gives you something else.
The asphalt surface takes no drainage coefficient. Its binder glues the stones, and a dense-graded mix's small voids don't connect, so water runs off the top instead of soaking through. Water still weakens the pavement, but it does it in the layers below, and that's where goes. With drainage in, this is the Handbook's AASHTO Structural Number Equation:
Layer 1 is the surface, 2 the base, and 3 the subbase, and the Handbook's version runs on the same way for more layers. Each is a thickness in inches, so a 1-ft layer goes in as 12. That makes three meanings of in this topic, after the degree of curve and traffic density. The Handbook uses the same letter for all three, and the equation around it tells you which one you have.
Sizing one layer
A design question runs the equation backward. It gives the required SN and every layer but one, and asks how thick that one must be. Subtract what the known layers supply, then divide what's left by what one inch of the missing layer buys: for the surface, for the base or subbase. For the base, that reads:
Then round up to the next half inch. Thicknesses are specified in half-inch steps, and a layer rounded down, even by a tenth of an inch, leaves the pavement short of the SN its traffic needs. So 13.1 in becomes 13.5, 13.6 becomes 14.0, and only an exact 13.5 stays put.
Drainage changes these answers too. Before the next two questions, find where and sit in the base equation above.
That's the base equation at work. sits in its denominator, so a wetter base buys less per inch and needs more inches, and shrinks the subbase's term on top, leaving the base even more to make up. Good drainage is structural capacity you don't have to pave.
An overlay makes up the difference
Pavements wear out. After years of trucks, the asphalt cracks and the base picks up fines and water, so the same layers no longer spread the load as well as they did when new. What they still supply is their effective structural number : the same equation, with each layer coefficient marked down to match the layer's condition. It comes from a condition survey or deflection testing, and a question gives it.
When the traffic forecast for the years ahead calls for a future structural number , a new asphalt overlay on top supplies the shortfall, and only the shortfall:
The overlay is new asphalt concrete, so it takes no drainage coefficient. Round up to the next half inch, as for any layer. The Handbook says nothing about overlays, so expect the question to tell you that the overlay's SN is the difference.